Cylinder Block Repair
Cast Iron Porosity DefectsCAUTION:
- Do not attempt to repair cracks.
- Do not attempt to repair areas where temperature will exceed 260° C (500° F).
- Do not attempt to repair areas exposed to engine coolant or oil.
1. Repair porosity defects with an epoxy sealer such as Devcon Aluminum Liquid F2 or equivalent.
1 Clean the surface to be repaired to a bright, oil free, metal surface.
2 Chamfer or undercut the repair area to a greater depth than the rest of the cleaned surface. Solid metal must surround the area to be repaired.
3 Apply the epoxy sealer and heat-cure with a 250 watt lamp placed 254 mm (10 inches) from the repaired surface or air dry for 10-12 hours at a temperature above 10° C (50° F).
4 Sand or grind repaired area to blend with the general contour of the surface.
5 Paint the surface to match the rest of the cylinder block.