Operation CHARM: Car repair manuals for everyone.

Two Color Dashboard - Paint Flaking


9232audi01

Group: 70

Number; 92-02

Date: 03/15/92


Subject:
Two-color Dashboard Paint Flaking


Model(s):
100, 100S, 1OOCS
M.Y. 1992


Condition

Inadaquate adhesion between PVC-slush foil and paint.


Production

Dyed two-colored PVC-slush foil introduced gradually as of February 1992


Service

According to the size of the damaged area, repair as follows:

1. Large areas of paint are flaking off on the entire surface

- Replace the dash

2. Paint flaking off - area no larger than 2mm in diameter

- Repaint with a fine hair touch-up brush.
- Clean damaged area with solvent
- Mix needed quanity of paint and hardener in the ratio 100 : 18
- Dab paint on with a fine hair brush

3. Paint flaking off - area larger than 2mm in diameter

- Repaint damaged areas
- Use tape to check adhesion of the paint surface surrounding the damaged area
- Clean with solvent
- Tape off attaching parts such as moldings, trim etc.
- Protect interior of vehicle against spray mist
- Mix needed quanity of paint and hardener in the ratio of 100 : 18


- To minimize spray mist as much as possible, use an air brush (nozzle size 0.8mm) or a spray gun with a nozzle of 1.5mm maximun
- Apply paint on the damaged area, let it dry for approximately 2 minutes and spray paint again
- Let paint dry at room temperature (in emergency cases only, drying could be accelerated by using a heater fan, maximum temperature 60~C/140~F)
- No pressure should be applied to the repainted area for at least 48 hours


Part numbers

L2K 769 3VY Al Platinum 200ml.

L2K 769 Q02 Al Ecru 200ml.

L2K 769 8RW Al Travertine 200ml.

ALZ 009 021 06 Hardener 500ml.

D 009 401 04 Solvent 250ml.


Caution

Before using any chemicals, carefully read the label on the container. Always follow all ot the manufacture's safety recommendations.